Hi,
In the BPV world, working with CMn steels you are often confronted with values as 15 lbs av. impact requirement with one testvalue not below 10lbs. I realised not to know for sure where these values origine from.
If you do, please let me know.

Thanks in advance.

Weldpartner
 
Replies continue below

Recommended for you

Hello Insult2Injury,

Thanks for your response. Ofcourse you're right.

Best Regards,

WeldPartner.
 
The CVN impact value requirements originated in various Codes of Construction, as well, in this case ASME B&PV Code, Section VIII, Div 1.
 
I followed the advise and I found indeed impact values, but..not for ASTM A106. Are there maybe referenced sources, from which an impact requirement of 15 lbs min. for ASTM A106 Gr B appears?

Thanks in advance.

 
Hello,

The answer reached me already: ASME VIII Div 1 UG 84 gives minimum charpy impact test requirements, for steeltypes with different yield strengths.

Please let me know if you have additional info,

Best regards.
 
WeldingPartner, various general material specs can list other values, such as in SA-20.

Specs for impact tested materials such as SA-350 will have their own values as well.

Otherwise, UG-84 is it.

Regards,

Mike

 
The 15 ft-lb criteria came from 1940s and 1950s research on brittle fracture related to the Liberty Ships built during WWII.

Joe Tank
 