Several years ago, we attempted a PQR on 13-8PH (or PH 13-8MO) and tensiles and bends failed miserably. The project was cancelled until now.
The history, as far as I can tell was that the original procedure called for:
Mat'l: PH13-8Mo Condition A
Process: GTAW
Filler: 1/16" PH13-8Mo
Joint Types: plate, V-groove, flat & vert
Preheat: 250F
Interpass: 550F
Shield Gas: Ar(20 CFH)/He(5 CFH)
Volts: 200
Amps: 24-28
PWHT: Solution H/T & Precip Age to H1050 (Method AMS 2759/3)
For the upcoming PQR my choices will be to use a ER630 filler; no preheat and watch interpass at 300F max; same PWHT. Other than that, I will turn down the amperage a litle bit.
Any other suggestions to improve success with my bend tests?
I am afraid that the condition H1050 is so hard that it will fail bends even if I do a perfect procedure. (bend tests IAW AWS methods)
Suggestions please.
Thankyou
The history, as far as I can tell was that the original procedure called for:
Mat'l: PH13-8Mo Condition A
Process: GTAW
Filler: 1/16" PH13-8Mo
Joint Types: plate, V-groove, flat & vert
Preheat: 250F
Interpass: 550F
Shield Gas: Ar(20 CFH)/He(5 CFH)
Volts: 200
Amps: 24-28
PWHT: Solution H/T & Precip Age to H1050 (Method AMS 2759/3)
For the upcoming PQR my choices will be to use a ER630 filler; no preheat and watch interpass at 300F max; same PWHT. Other than that, I will turn down the amperage a litle bit.
Any other suggestions to improve success with my bend tests?
I am afraid that the condition H1050 is so hard that it will fail bends even if I do a perfect procedure. (bend tests IAW AWS methods)
Suggestions please.
Thankyou