Has anyone experience of getting A320 L7M bolts to achieve the specified minimum toughness values at -120 deg C?

Steve Jones
Materials & Corrosion Engineer
 
I believe these are rated to -40C, not -120C which is a cryogenic application.

Alternatives NACE material for the stud would be ASTM A193 L7M with the ASTM A194 2HM nut.

Kenneth J Hueston, PEng
Principal
Sturni-Hueston Engineering Inc
Edmonton, Alberta Canada
 
Whereas the impact test temperature for L7M is -100F (-73 C), your chances of finding L7M meeting the required energy absorbed values at -150C are nil based on old impact test data that I've seen.

 
Why would the bolts be in H2S service, are they inside the piping and vessels?
 
No - they are externally located but are still to meet the requirements of ISO 15156.

Steve Jones
Materials & Corrosion Engineer
 
SS304L is commonly used in Cryogenis Environments, also you could have them coated in PTFE or Xylan/Xylar. Don't know if this is any help?
 
We're going the ISO 10423 route and trying ASTM A453 Gr660 Class D. Fingers crossed on the Charpy tests.

Steve Jones
Materials & Corrosion Engineer
 