91RepairGuy
Mechanical
Our company recently needed to increase our thickness range for manually welding P1-P1. We used 1.5" thick SA-516 plate with a 37.5-10 degree compound bevel for the test coupon. The root passes were welded with ER70S-B2 using GTAW, 3/4" deposited metal thickness. The balance was welded with E7018 using SMAW, 3/4" deposited metal thickness.
The following data was recorded:
Position of Groove: Flat 3G
Weld Progression: Uphill
Preheat: 200F
Interpass: 600F
PWHT: 1150F +-25F
Time: 1.5 hrs
Rate above 600F: DNE 250F/hr
Shielding gas: 99.9% argon
Current: direct
Polarity: GTAW-str, SMAW-rev
Amps: Root 100-150, Cover 110-175
Technique: Root-stringer, Cover-weave
Electrodes: single
The coupon was completed and sent out for PWHT and destructive testing. Failure of the GTAW portion was discovered while performing side bends and no tensile pulls were performed. The SMAW portion appeared to be satisfactory with no visible defects. The GTAW portion had multiple separations, approximately 1/8" wide. Many of these defects were parallel to each other and stacked two high (seems to be consistent with the location of the stringers in the root pass). Each weld pass was power cleaned with a new wire wheel.
No visible indications were visible in the parent metal, although defects are present in the weld metal, adjacent to the parent metal. I have photos available for analysis.
Is there an issue with depositing 3/4" GTAW weld metal thickness? Would you recommend a minimum number of GTAW passes when the procedure is re-qualified? We would like to understand what happened to cause the multiple defects in the GTAW portion of the weld. Your assistance is greatly appreciated
The following data was recorded:
Position of Groove: Flat 3G
Weld Progression: Uphill
Preheat: 200F
Interpass: 600F
PWHT: 1150F +-25F
Time: 1.5 hrs
Rate above 600F: DNE 250F/hr
Shielding gas: 99.9% argon
Current: direct
Polarity: GTAW-str, SMAW-rev
Amps: Root 100-150, Cover 110-175
Technique: Root-stringer, Cover-weave
Electrodes: single
The coupon was completed and sent out for PWHT and destructive testing. Failure of the GTAW portion was discovered while performing side bends and no tensile pulls were performed. The SMAW portion appeared to be satisfactory with no visible defects. The GTAW portion had multiple separations, approximately 1/8" wide. Many of these defects were parallel to each other and stacked two high (seems to be consistent with the location of the stringers in the root pass). Each weld pass was power cleaned with a new wire wheel.
No visible indications were visible in the parent metal, although defects are present in the weld metal, adjacent to the parent metal. I have photos available for analysis.
Is there an issue with depositing 3/4" GTAW weld metal thickness? Would you recommend a minimum number of GTAW passes when the procedure is re-qualified? We would like to understand what happened to cause the multiple defects in the GTAW portion of the weld. Your assistance is greatly appreciated