Hello all, I was wondering if there is a specific reason customers ask foundries for Ni (1-2%) in low alloy steel castings to improve weldability? We know Ni is good for low temperature toughness but not sure what is the effect on weldability.
 
Replies continue below

Recommended for you

Toughness aside, Ni has little affect on the weldability of various steels based on review of the carbon equivalency formulas. Nickel and even copper have a high denominator in the CE formula's, which means they have little impact on precautions necessary for welding.

 
Exactly, but adding more Ni would only increase the CE so why want more Ni if you have met the toughness spec?
 
Because Ni does help with increasing hardenability of the casting, which helps for heat treatment (quenching) of thick section castings.
 
What grade of castings ASTM 148 ? Some manufacturers maintain 1.5% Ni with 0.3%Mo. I use lower quantities of Ni and increase Mn up to 1.2% with some grain refiners. It is a matter of choice and experience. Apart from this grade, I have no knowledge of Ni being added in low alloy steel castings.

I'm just one step away from being rich, all I need now is money.
( read somewhere on the internet)
 
That's right, adding Mn, Cr and Mo should be able to take care of the hardenability (better effect than Ni anyways).
Thanks!
 
You can count on arunmrao as our metal foundry expert.
 
In terms of steel hardenability, nickel is a pretty benign alloy addition, which is reflected in various carbon equivalent formulae. Its primary effect is grain refinement, a strengthening mechanism that also improves low temperature fracture toughness.
My background is welding, and I consider 1Ni-¼Mo to be the "sweet spot" for a low alloy filler metal composition with all-round good properties.

"If you don't have time to do the job right the first time, when are you going to find time to repair it?"
 