Eng-Tips is the largest forum for Engineering Professionals on the Internet.

Members share and learn making Eng-Tips Forums the best source of engineering information on the Internet!

  • Congratulations dmapguru on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

When is Lamellar Tearing a concern?

MSL93

Structural
Joined
Aug 10, 2017
Messages
6
Location
US
I have seen an uptick in customer specifications that state the need to do ultrasonic testing to check for lamellar defects in steel plates. The specifications will generally be vague on the details for what constitutes what needs to be tested. For example, they will say things like "Plates subject to high, localized through-thickness strain" but not list any criteria for what constitutes what is considered "high" or "thick plates subjected to bending stresses" but not list any criteria of what a thick vs. non-thick plate is (greater than 1" thick, greater than 2" thick, etc.).

My question is does anyone know of any good references that I can look into to fill in the knowledge gap here to better understand how to apply these customer specifications?
 
I ran into this once before and was satisfied by the AISC Commentary on the subject. Ended up dog-earing a triaxial weld to avoid the issue.
 
1742575693562.png

I thought the problem was found with very large thicknesses, say 80 mm, but the attached diagram suggests it could be much less.
 
As a parallel, I think "cracking" was thrust into the limelight relatively recently due the the San Francisco Transit Center fiasco. The plate-girder/built-up node had cracks propagating from welded joints at thick plates. I've noticed greatly increased Charpy V-notch testing requirements lately on contract documents from the engineering corporation that designed the failed connection.

 
This is the summary research paper that I read when I was in college. It was published in 1973, but my professor still thought it was relevant in 1995-ish when I took that class. In particular it shows a number of examples of details that are susceptible to lamellar tearing versus ones that are "improved".


I should point out that a lot of this is essentially written into the our pre-approved moment details.... At least since the Northridge based revisions to increase ductility. I'm talking about the rat holes, back gouging and such. A good welder that knows how to properly sequencing his (or her) weld passes or buttering the joint before.

It's all about how through-thickness strains can be brittle when that strain is overly restrained. This should be more common with thicker plates because of the thicker welds they require.
 
This paper is definitely still relevant....still in the bibliography of CSA W59 Annex Q along with other valuable references.
 
The Welding Institute has a good basic reference and guide.

The threshold for 'problematic thickness' will vary depending on the degree of restraint, the type and size of weld and even whether preheat is used.

EN 1993-1-10 Material toughness and through-thickness properties is the relevant Eurocode standard.
PD 6695-1-10 Recommendations for the design of structures to BS EN 1993-1-10 is linked from the National Annex and has a simple checklist to determine whether a higher 'Z-quality' steel is required (more ductility in the Z-direction).
 
Last edited:
In the industry I am in (utility), I see many spec's that have this requirement in them for any plates that are 1-1/2" thicker or greater and subject to any through-thickness stress.

We also always take exception to this (and are usually successful). We have never once found a plate with an issue when we have performed the UT testing. Here is a response we received from Larry S. Muir with AISC (back in 2019 I believe) regarding the topic:
I cannot provide a date when lamellar tearing became a less significant issue in our industry, but your general perception is correct. It is much less of an issue than it once was. I have worked in the steel industry for over twenty years, and I have never personally been involved with a project where lamellar tearing occurred. I have only heard of a couple potential instances of lamellar tearing over that time period.

The following statements in AISC documents support the idea that lamellar tearing is less of an issue today than it once was:

• Section 5.4 of AISC Design Guide 21 (a free download for members from
http://www.aisc.org/dg)
addresses lamellar tearing and states, “Current steel-making practices have helped to minimize lamellar tearing tendencies. With continuously cast steel, the degree of rolling after casting is diminished. The reduction in the amount of rolling has directly affected the degree to which these laminations are flattened, and has correspondingly reduced lamellar tearing tendencies… The incidence of lamellar tearing today is significantly reduced as compared to the past, due mostly to proper joint selection and better steel chemistry.”

• The Manual states, “Although lamellar tearing is less common today, the restraint against solidified weld deposit contraction inherent in some joint configurations can impose a tensile strain high enough to cause separation or tearing on planes parallel to the rolled surface of the element being joined… Dexter and Melendrez (2000) demonstrate that W-shapes are not susceptible to lamellar tearing or other through-thickness failures when welded tee joints are made to the flanges at locations away from member ends.”

Neither the 2016 Specification nor its Commentary mentions lamellar tearing. There is no requirement in the Specification to UT the base metal. There are requirements to UT CJP welds in Section N5.5. There are also toughness requirements in Sections A3.1c and 1d.
Section J6.2c of the Seismic Provisions includes requirements to UT base metal in some instances. There are no pre-fabrication UT requirements and the post-welding requirements apply only to specific conditions. It states, “After joint completion, base metal thicker than 1½ in. (38 mm) loaded in tension in the through-thickness direction in T-and corner-joints, where the connected material is greater than ¾ in. (19 mm) and contains CJP groove welds, shall be ultrasonically tested for discontinuities behind and adjacent to the fusion line of such welds. Any base metal discontinuities found within t/4 of the steel surface shall be accepted or rejected on the basis of criteria of AWS D1.1/D1.1M Table 6.2, where t is the thickness of the part subjected to the through-thickness strain.”


While the Specification for Safety-Related Steel Structures for Nuclear Facilities does not contain UT requirements for base metal, it does acknowledge that the engineer of record may wish to impose project-specific requirements. Section NA3.1d states, “The project specification covering material for structural components that, as a result of proposed welding procedures, design details, etc., are susceptible to lamellar tearing shall, as determined by the engineer of record, include the requirement that the material shall be either ultrasonically examined in accordance with ASTM A578/A578M, Level C, or tested in tension in the through-thickness direction (z-direction). The resulting percentage reduction in area in the z-direction shall not be less than 90% of that in the direction of material rolling.” A User Note states, “In determining the need for prefabrication inspection and the inspection acceptance level, the engineer should consider the geometry of the joint, the material type and grade, the anticipated quality of the material, and other experience factors. See Chapter NN. Lamellar tearing is generally caused by the contraction of large metal deposits with high joint restraint; lamellar tears seldom result when weld sizes are less than ¾ in.”

I also recently worked with a colleague and an individual working at a U.S. mill to write the following for an article that may be published in the near future:

“Lamellar tearing is one consideration related to this anisotropy. Several factors play a part in lamellar tearing, including joint configuration and steel chemistry. The manufacturing process itself also plays a role. The current steel making practice of continuous casting places demands on the producer that have the benefit of controlling the shape of inclusions and improving through-thickness strength. Therefore current continuous cast products have less likelihood of lamellar tearing than older ingot cast product did. Engineers can reduce the likelihood of lamellar tearing through good design practice, as described in Design Guide 21. Material specifications define some aspects of chemical composition, such as limits on sulfur, which can be objectively evaluated assuming the proper expertise, but the details of the manufacturing process may be more difficult to know and to evaluate.”
 