2
I have to do a fillet weldment between a 2" thickness 17-4ph H1025 plate and a 1 1/2" A36 or 44W plate. Weldment profile is 5/16" wide. I have to elaborate procedure and I'm looking for the better filler metal.

Should I weld on annealed plate and is it safe to make heat treatment (conditioning H1025) after all welding?
 
Replies continue below

Recommended for you

What is the weld joint configuration? Also, is this a structural weld (load-carrying)? You have a significant strength mismatch between the 17-4PH H1050 and A 36.
 
Since the failure would be in the CS you had might as well weld with CS filler. It doesn't matter how strong the joint is.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
T joint is the configuration. At first sight, I have choice between a 309 grade or a CS filler metal but, would these material could cause chemistry problems ? Should I weld annealed ? Before or after H1050 conditionning ?
 
Yes, weld the 17-4 in the annealed condition, and age after welding at H1025. This will establish bulk properties in the 17-4 and provide stress relief for the CS. Use 309 filler metal.
 
Do you care about the heat treat condition of the CS?
If not then anneal the 17-4 before welding, and age the whole thing after welding.
You could use 309 for filler, or 17-4, or CS.

= = = = = = = = = = = = = = = = = = = =