I found a W-322 Precipitation Hardenable SS in Source Book on Stainless Steels, ASM, p. 394 (1976). Info source: Metal Progress Databook, Mid-June 1975.
W-322
Mfr.: Simonds Steel Div., Wallace-Murray Corp.
Typical composition: 0.07 C, 17.0 Cr, 6.75 Ni, 0.2 Al, 0.8Ti
ASTM or AMS spec.: no
Yield strength: 75,000-210,000 psi
Tensile strength: 125,000-225,000 psi
Elongation: 8-15%
Hardness: C22-46
Typical applications: Valves, bearings, rollers, cams, pump parts.
The max. strengths & hardness are presumably for the precipitation-hardened condition.
If necessary to heat-treat, first try to verify the composition; then, if no other data, try using the procedure for 17-7PH in MIL-H-6875H.