Please can anyone suggest how I can continuosly separate the fines 15 microns or less from a (50-120gpm) clay slurry with a PSD of 2-45 microns I have tried Hdrocyclones but their operation seems to seperate based on a flow ratio between the underflow and the overflow instead of Particle size and this peice is stalling my project and stressing me out real bad
Help in needed
Thanks
 
Try doing a search on "Elutriation" especially as it relates to mining and mineral industry.
 
Schweitzer's Handbook of Separation Techniques for Chemical Engineers -McGraw-Hill- has chapters of centrifuging and hydrocyclones, that may be helpful. The latter has graphs and tables for selecting and sizing hydrocyclones for particular duties (flow rates, particle sizes, etc.).
 
we were using a combination of flocculants and decanter centrifuge very successfully for a similar task.
M777182
 
Hydrocyclones are the way to go. Yes they will send a lot of water to the overflow, along with the -15 micron material.

In general they are combined with a thickener to recover water from the cyclone overflow stream. Very common for fines removal in mineral sands operations.

General rules of thumb:

Higher pressure = finer cut point
Lower feed slurry density = finer cut, better separation efficiency.
Smaller cyclone = finer cut

Contact Warman, Krebs, Linatex or Multotec for further design info.
 