Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Regarding composite failure [fiber or matrix] in nastran/patran

Status
Not open for further replies.

Abi786

Aerospace
Joined
Nov 17, 2015
Messages
15
Location
KR
Dear All

Greetings

I have a very basic question regarding composite failure analysis


I am using Tsai-Wu failure criteria, Solution seq-101, shell elements
i can determine Failure index and stresses in elements


My question is

I want to know is the failure is because of matrix or fiber? how can I ?
how to determine fiber failure and matrix failure in certain ply?
A little explaination will be very helpful

Advance thanks
AB

 
Tsai-Wu and similar criteria don't have details of the failure. You can look at each component of the criterion for clues and it pays to recover the three basic (1, 2 and 12) stresses and strains in each layer. If the layers are UD carbon/polymer then it will usually be clear what is likely to be breaking first in the layer which is predicted to be failing, fiber or matrix. The components of Tsai-Wu have to be recovered manually (or in a spreadsheet), so it's often easier to output the basic stresses and strains.

If your fiber is not carbon then it will likely be less clear. It will also depend on how brittle the matrix is. Glass has a tensile strain to failure of between three and four percent, which is close to many polymers, although it is likely to exceed them a bit.

It can also be hard with woven material. With cloth/polymer essentially in-plane shear close to the allowable is an indication of matrix failure. BUT, with cloth if the fiber is carbon it can be harder to tell than if it's glass, as carbon's in-plane shear failure stress can be close to that of a matrix resin, although it is usually higher. HS and IM carbon can be assumed to have a shear strength of 17 ksi/120 MPa (this is old Amoco data), annoyingly close to many polymers. Glass's shear strength should be in excess of 200 ksi or 1300 MPa (glass fibers are more-or-less isotropic and will have a shear strength above 50% of the tensile strength, and UTS is probably between 2200 MPa and 2800 MPa).

There are a few ways to keep an eye on matrix and fiber separately but none work well (you can model a layer of resin separately from a layer of fiber but this sort of thing has a lot of drawbacks).

Keeping the three basic stresses and strains for each ply available is sensible, usually pretty easy and passably useful, especially for UD carbon/polymer. (It also hays to keep an eye on through-thickness shear, which is usually available, certainly with Nastran and PCOMPs/CSHELLs, which I assume you are using from your mention of a 'solution sequence 101'.)
 
D'oh! Not only is this the Nastran forum but you mention it in your post's title. Well, it's Friday.
 
1) Tsai-Wu or any other interactive failure criteria is not a good choice. They don't correlate to test data. See previous posts here and on Composite engineering and Aircraft engineering forums
2) There is no simple, accurate, definitive method to determine the failure mode from an interactive theory FI. It just stirs everything into one equation (and outputs a meaningless number).
 