For those that are interested, there are two ASME B&PV Code Cases (2179-3, and 2180-2) that will be revised to reflect changes in the allowable stress values. These Code Cases pertain to the following materials 9Cr-2W and 12Cr-2W (Grade 92 and Grade 122, respectively). The changes in allowable stress are for the following service temperatures;
Code Case 2179-3 (Grade 92)
Revised Tube Stress column, other column is now Forgings, Pipe and Forged Pipe
Original stress lines
Tube
1050 deg F 17.2 Ksi revised to 16.1
1100 deg F 13.6 revised to 12.3
1150 deg F 10.2 revised to 8.9
1200 deg F 6.9 revised to 5.9
Forgings, Pipe and Forged Pipe
1050 deg F 16.6 revised to 15.7
1100 deg F 13.0 revised to 12.0
1150 deg F 9.6 revised to 8.6
1200 deg F .... revised to 5.6
For Code Case 2180-2
1050 deg F 16.8 Ksi revised to 14.4
1100 deg F 12.9 revised to 10.6
1150 deg F 9.3 revised to 7.2
1200 deg F 6.2 revised to 4.5
Also, the cast version of Grade 92 material is winding thru the Code committees.
Code Case 2179-3 (Grade 92)
Revised Tube Stress column, other column is now Forgings, Pipe and Forged Pipe
Original stress lines
Tube
1050 deg F 17.2 Ksi revised to 16.1
1100 deg F 13.6 revised to 12.3
1150 deg F 10.2 revised to 8.9
1200 deg F 6.9 revised to 5.9
Forgings, Pipe and Forged Pipe
1050 deg F 16.6 revised to 15.7
1100 deg F 13.0 revised to 12.0
1150 deg F 9.6 revised to 8.6
1200 deg F .... revised to 5.6
For Code Case 2180-2
1050 deg F 16.8 Ksi revised to 14.4
1100 deg F 12.9 revised to 10.6
1150 deg F 9.3 revised to 7.2
1200 deg F 6.2 revised to 4.5
Also, the cast version of Grade 92 material is winding thru the Code committees.