No. You could, however, by qualifying on a 1.5" thick material. Time at temperature is a supplementary essential variable when impact testing is required. It is not an essential variable otherwise.
Your PQR qualifies for 5 mm to 50 mm base metal thickness and a maximum of 50mm deposited weld metal thickness
For welding 200mm base metal you need a PQR done on a minimum of 1.5" thick base metal with deposited weld metal of each process of ¾" or more.
If you take a 1.5" thick base metal and weld it with 2 processes (¾" each), you will qualify for base metal of 5 to 200mm and deposited weld metal for each process of 200mm. Refer Table QW-451.1 of Section IX