Hello, this maybe a silly question, and sorry for my english.
I have a PQR for double process GTAW & SMAW (refer picture) with 10.97MM base metal. Can i produce WPS for GTAW process with 1.5mm-6mm base metal qualification base on my GTAW/SMAW PQR?
1000133126.jpg
 
Yes, if the Code has not changed in the past 10 years.
 
Karabau,
Do not confuse base metal qualified with weld deposit qualified
As per Table 451.1 your base metal qualified is 5 mm - 21.94 mm
Maximum GTAW deposit is 6 mm.

Unless I have misinterpreted that 10.97 mm is greater than 10 mm (Interpretation ?)
 
Your construction code (which you haven't specified, such as B31.3 or VIII-1) may set additional, more stringent requirements on top of ASME IX. Take those into consideration as well.
 
Wouldn't you need to test the GTAW passes without the others to qualify that?
But you sure could use the same procedure.
 
I may be reading your post wrong, but if your current PQR were completed with a 10.97mm thickness, the range of qualified thickness would be 4.7mm - 21.89mm. You would need to do a PQR with a 1.5mm thickness, and that will only give you a qualified range of 1.5mm - 3mm
 
Hello, this maybe a silly question, and sorry for my english.
I have a PQR for double process GTAW & SMAW (refer picture) with 10.97MM base metal. Can i produce WPS for GTAW process with 1.5mm-6mm base metal qualification base on my GTAW/SMAW PQR?
View attachment 7184
Basically No - if your original PQR was on any thickness 10 mm or below you could write a WPS for 1.5 to 6 mm
 
Hello, this maybe a silly question, and sorry for my english.
I have a PQR for double process GTAW & SMAW (refer picture) with 10.97MM base metal. Can i produce WPS for GTAW process with 1.5mm-6mm base metal qualification base on my GTAW/SMAW PQR?
View attachment 7184
The final answer : No.
under the requirement of ASME Section IX (QW-200.4) :

" When following a WPS that has more than one welding process, filler metal, or set of variables, each process, filler metal, or set of variables may be used individually or in different combinations, provided :
(1) the essential, nonessential, and required supplementary essential variables associated with the process, filler metal, or set of variables are applied
(2) the base metal and deposited weld metal thickness limits of QW-451 or Table QW-453, as applicable, for each process, filler metal, or set of variables are applied
 

Part and Inventory Search