Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations TugboatEng on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Property range for tensile and 1026.

Status
Not open for further replies.

EngineerDave

Bioengineer
Joined
Aug 22, 2002
Messages
352
Location
US
Alot of sources are reporting just a minimum range for the tensile strength of 1026. Do you know any source to find a suggested range for tensile and yield, instead of just a minimum.

I have searched alot of sources, including Mil handbook and Metals Handbook. They all appear to report the minimum tensile of 1026 and not a range.

 
As you already know, strength depends on thermomechanical processing, chemistry, etc. Some additional data to the minimums that you already have:

Hot-rolled wire from electric arc furnace
two cooling rates-- fast & slow

Fast - yield = 43 ksi (295 MPa), tensile = 74 ksi (510 MPa), elongation = 30%

Slow - yield = 45 ksi (310 MPa), tensile = 80 ksi (550 MPa), elongation = 25%

This data is from a U.S. domestic steel mill, listed as typical. Most 1026 is used for tubing or bars, this data may not be of much value if you require properties for cold-drawn bars.
 
dont have 1026 in my Guide to Engineered Materials.... (AMP December 2001)

But I do have 1022 and 1030:

SAE 1022: SAE 1030:
As Rolled (hot rolled):
UTS: 73ksi 80ksi
Yeild: 52ksi 50ksi
Elong: 35% 32%
Area Reduc: 67% 57%
Brinnel Hard: 149 179
Izod Impact: 60ft*lbf 55ft*lbf

Normalized at 1700F:
UTS: 70ksi 76ksi
Yeild: 52ksi 50ksi
Elong: 34% 32%
Area Reduc: 68% 61%
Brinnel Hard: 143 149
Izod Impact: 87ft*lbf 69ft*lbf

Annealed at 1600F:
UTS: 65ksi 67ksi
Yeild: 46ksi 50ksi
Elong: 35% 31.2%
Area Reduc: 64% 58%
Brinnel Hard: 137 126
Izod Impact: 89ft*lbf 51ft*lbf


I think that several of the values above are wrong:
yeild for 1030 all coditions. (shouldn't this be higher than 1022?)
Izod Impact for 130 annealed condition. (shouldnt the impact energy absortion increase for annealed steel?)

Hope this Helps!


Nick