I am in need of some temperature data for Level 4 Coldworked Nitronic 50. What is the tensile and yield strength of Nitronic 50 at 400 degrees F. Are there any temperature lists available for this material. I appreciate any pointers.

Thanks Chris
 
Get it from AK. If they don't have it you won't find it.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
I'll give it a try.

Thanks
 
Oh Ed, yee of little faith. You forgot there are lots of old timers that have lots of old data.

I have old, old Armco data on Nitronic 50 that shows the following for 54% cold swaged

Temp UTS YS
RT 230 216
200 215 205
300 206 199
400 200 194
500 195 191
 
You can also look the data up under 22-13-5 SS or XM-19.

If I recall correctly the numbers posted by MikeMet are for small diameters. We used 135 UTS as the practical max for anything above 1 1/2" in diameter
 