Nil Ductility Temperature or Ductil to Brittle Transition Temperature

Status
Not open for further replies.

commocheck

Mechanical
Mar 17, 2006
4
Does anyone know where I can locate the NDTT or DBTT (Nil ductility or ductil to brittle transition temps) for 174-h900?

Thanks
 
Replies continue below

Recommended for you

I meant to write 17-4 h900, instead of 174-h900. Sorry for the mix up.
 
I couldn’t locate specific impact energy data below room temperature in the literature I have for 17-4PH in this heat treatment condition. At room temperature, the value reported is about 20 ft-lbs minimum CVN impact energy at the 900 heat treatment condition*. Below room temperature, the impact energy for this heat treatment condition is going to decrease in value so if there is a so-called DBTT it might be above RT, if you can find CVN data at elevated temperature.

*Source; "Handbook of Stainless Steels" by Peckner and Bernstein
 
Many thanks. This is exactly the info I've been looking for.
 
From Armco 17-4PH

H900 CVN Ft-lb
75F 19 ft-lb
32F 18-20 ft-lb
-40F 7-9 ft-lb
-80F 8 ft-lb
-320F 3-4.5 ft-lb


 