Nickel Plating on 9Ni-4Co-0.3C Steel HT 220-240-KSI [Acft engine mount parts].

Status
Not open for further replies.

WKTaylor

Well-known member
Joined
Sep 24, 2001
Messages
4,320
Location
US
Help! I have a bizarre problem.

Our 9Ni-4Co-0.30C steel alloy parts [HT220-KSI] [turbine engine aft mount] have a 0.0035--0.0055" thick nickel plating per BAC5746 applied to ~80% of the surface area.

BAC5746 requires post plating hydrogen embrittlement [PPHE] relief bake at 375F+/-15F for 23-hours min, which is in-line with other PPHE relief bakes for nickel plated HS steel parts [AMS2759/9, etc]. However, drawing notes for each of these 9Ni-4Co-0.30C steel parts EXPLICITLY requires PPHE relief bake at 475F+/-15F for 24-hours min.

We are now in the overhaul process of stripping-off the nickel plate, inspecting, repairing [corrosion, etc] and then re-plating.

Serious problem: our plating shop, like MOST plating shops, has capability to accurately PPHE bake at 275F+/-15F or 375F+/-15F... but these same ovens cannot reliably bake the parts at 475F+/-15F.

Unfortunately there is NO tech data available to explain why 475F bake was chosen. Soooo... I have beaten-up our local M&P guys for a real answer as to "why the 475F bake?", but have gotten a general [unsatisfying non-scientific] response: "because the drawings say-so".

A higher level [corporate] M&P plating expert thought that MAYBE there was a hydrogen diffusion-path issue, due to the [high density] deep plating thickness and large surface area coverage; so, perhaps, the extra temperature bump [100F] was needed to drive the hydrogen to bare steel areas within a reasonable time frame [24-hrs]. Another thought proposed was that the extra temperature would harden/densify the nickel plating, along with PPHE relief... but 450F seems a little low for that purpose.

NOTE.
The Corporate M&P engineer was quite disturbed that we would rely on nickel plating for corrosion protection of steel parts that could see extreme service temperatures up-to 850F: depending on the reference, max service temp for Nickel plate is either 700F or 800F.

Any experience along these lines out there??? PLEASE ADVISE!!!

Regards, Wil Taylor

Trust - But Verify!

We believe to be true what we prefer to be true.

For those who believe, no proof is required; for those who cannot believe, no proof is possible.
 
Nickel coatings that contain phosphorus will form Ni3P precipitates in the range of 420 to 500 F. However, electrodeposited nickel from sulfamate baths typically do not contain P. So, I can only surmise that the reason for the elevated temperature is for enhanced embrittlement relief of a large component with a thick coating.
 
Status