May 24, 2007 #1 jlcochran1 Mechanical Joined Oct 30, 2003 Messages 94 Location US Welding a replacement section of a pressure vessel. Monel 400 to 316L SS. Looking for any GMAW wire recommendations. 1/4" Monel to 3/8" 316L SS.
Welding a replacement section of a pressure vessel. Monel 400 to 316L SS. Looking for any GMAW wire recommendations. 1/4" Monel to 3/8" 316L SS.
May 24, 2007 #2 weldtek Materials Joined Feb 12, 2005 Messages 897 Location US Suggest you contact the technical folks at Special Metals, but I think you could use (1)82 or Inco A. Upvote 0 Downvote
Suggest you contact the technical folks at Special Metals, but I think you could use (1)82 or Inco A.
May 24, 2007 #3 weldtek Materials Joined Feb 12, 2005 Messages 897 Location US Sorry you did say GMAW, ERNiCr-3 ( 82) should work. Upvote 0 Downvote
May 24, 2007 #4 stanweld Materials Joined May 9, 2003 Messages 2,906 Location US There are a number of nickel base weld filler metals that can be used. You need to determine the corosion compatabilty of the materials before selecting the appropriate one. Upvote 0 Downvote
There are a number of nickel base weld filler metals that can be used. You need to determine the corosion compatabilty of the materials before selecting the appropriate one.