Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations MintJulep on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Low Magnetic Permeability when welding 316L

Status
Not open for further replies.

MikeMech

Mechanical
Joined
Nov 29, 2000
Messages
92
Location
US
We have an ongoing job that requires welding 316L base metal with 316 alloy. Magnetic permeability of the entire finished weldment must measure less than 2.0mu on a Severn Gage.

Our customer supplies the base metal, we do the welding. We have had infrequent but recurring problems over the years with seemingly random welds failing the 2.0 permeability test. The welding and testing is being performed by a competent, experienced individual. Why is this happening? How can we best ensure low magnetic permeabilty?

My current theory is as follows: Magnetic permeability is proportional to ferrite percentage/ferrite number. The base metal and filler metal chemistry ranges specified could result in an unacceptable ferrite percentage if the Nickel Equivalent is at the low end of the allowable range and the Chromium Equivalent was at the high end of the acceptable range. A Schaffer-DeLong type diagram indicates this. Statistically, this is unlikely in any particular instance but probable over the long run. My first attempt at a "silver bullet" fix would be to purchase only filler wire with very low, but still within allowable tolerance, ferrite numbers.

I will be performing some experiments with 316 filler metals having ferrite content throughout the allowable standard range. Any advice on weld procedure improvements to try that may help? Annealing after welding is not an option, nor is changing the material.

Comments appreciated!

Thanks,

MikeMech
 
Can you weld it with alloy 82/182 (Inconel)? Otherwise, you're on the right track, but watch out for weld cracking.

Gold is for the mistress - silver for the maid
Copper for the craftsman cunning in his trade.
"Good!" said the Baron, sitting in his hall
But iron - cold iron is the master of them all.
Rudyard Kipling
 
MikeMech;
I would agree with your approach, there is not much you can do regarding the welding procedure.
 
Metalguy,

We are stuck with 316 alloy for now. The frustrating thing is that everything comes out fine 95% of the time...
 
Status
Not open for further replies.