Dear all.
I want to weld dissimilar materials: copper (Cu) and 316L stainless steel using the TIG welding process. what type of electrode and filler rod are suitable? thank you for your answer.

Regards
 
Replies continue below

Recommended for you

Not a winner, the two materials won't fuse properly, but instead form intermetallic bonds that are weak.

It's possible to make a brazed joint work, using a silver-based braze alloy. It's possible to purchase an explosively formed tube junction (bimetallic tube coupling) and weld each side of it to the mating material. I think you would be more likely to find aluminum/copper junctions and aluminum/stainless junctions, i.e. making 3 welds to join the tubes.
 
ERNi-1 if you must weld. Other alloys will work, you need <65% nickel. I prefer brazing in this case.
 
several articles were carried out using ErNi-3 welding wire/filler rod for TIG. What is the difference with ErNi 1 and ErNi-3? I weld plates with a thickness of 3 mm Cu and SS 316L.
 