Apr 2, 2001 #1 kstaylor Mechanical Joined Jan 8, 2001 Messages 86 Location US Does anybody have a sure-fire way of de-Gaussing a piece of 9Cr-1Mo pipe in order to make a GTAW weld? The section of pipe is magnetic and plays havoc with the arc from the Tig torch!
Does anybody have a sure-fire way of de-Gaussing a piece of 9Cr-1Mo pipe in order to make a GTAW weld? The section of pipe is magnetic and plays havoc with the arc from the Tig torch!
Jun 8, 2001 #2 Rich2001 Mechanical Joined Mar 23, 2001 Messages 896 Location US Use a single or if more power is required yorks from a magnetic particle tester., Use AC put on and pull off. Several times may be required. Rich Upvote 0 Downvote
Use a single or if more power is required yorks from a magnetic particle tester., Use AC put on and pull off. Several times may be required. Rich