Eng-Tips is the largest forum for Engineering Professionals on the Internet.

Members share and learn making Eng-Tips Forums the best source of engineering information on the Internet!

  • Congratulations JStephen on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Axle failure, thoughts 9

Status
Not open for further replies.

4130 metalworks

Mechanical
Joined
Sep 22, 2024
Messages
5
Location
AU
20240926_211622_bquzkm.jpg
20240926_211609_vgjrff.jpg
20240926_211704_uuvgln.jpg


Hi, I'd like to get the groups thoughts on why this axle shaft failed and how to best go about testing the rest of them. The shaft is heat treated 4140, from machining the splines the hardness seems to be the outer 2-3mm.
Unfortunately I don't have much information from the manufacturer to go with

The vehicle is reasonably heavy but low powered and was travelling at speed when this happened

Thanks in advance for any help
 
1. Check whether the hardness is in correct range.

2. Take a torsional rigidity text in a simulated aseembly condition (if test cost is not in consideration), compare result with theoretical value.
 
6k!? What is the test scope? 1k to slice and do a simple case depth survey of a couple slices should be more than enough. Do one far away from fracture surface and one right beside.

Friction could have heated it up to austenitizing temp and then you end up with brittle surface to fracture and start cracking.

Looks like fatigue on bigger OD fracture donut with rapid fast fracture failure of centre circle.

Replace with 4330V 150ksi min yield and Gas FNC. Should be invincible compared to this. Cost increase of material is not much. Gas FNC is cheap.
 