In accordance with API 6A, the size of a TC or a QTC for a part shall be determined using the ER method give in 5.7.2. What is exactly the method ER? Could you give me an example?
 
Replies continue below

Recommended for you

It is explained in API 6A, Section 5.6.2 Equivalent Round (ER). There are equations to calculate ER.

If you review API 6A they even provide a definition under Terms and Conditions

3.1.41
equivalent round ER
standard for comparing various shaped sections to round bars, in determining the response to hardening characteristics when heat-treating low alloy and martensitic corrosion-resistant steel

The reason for the above is that hardenability curves during quenching, like Jominy Curves were performed using round bars as a standard.

 
As far as I understand, ER is mainly used to determine the size of the test coupon during heat treatment process.

Different shapes will have different ER and this will come handy during QTC.