Dec 9, 2010 #1 qcrobert Industrial Joined Jun 24, 2010 Messages 229 Location US Wondering if anyone here has had any experience with welding 310 material to G-30 hastelloy material. If so, what SMAW filler metal did you use? Thanks, Robert
Wondering if anyone here has had any experience with welding 310 material to G-30 hastelloy material. If so, what SMAW filler metal did you use? Thanks, Robert
Dec 9, 2010 #2 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US qcrobert; My question back to you is what is the intended service of this dissimilar metal weld joint? Corrosion at elevated temperature? Upvote 0 Downvote
qcrobert; My question back to you is what is the intended service of this dissimilar metal weld joint? Corrosion at elevated temperature?
Dec 9, 2010 Thread starter #3 qcrobert Industrial Joined Jun 24, 2010 Messages 229 Location US It is for elevated temperature to weld 1/4" 310 angle clips (that hold insulation) to G-30 Hastelloy base metal. My thoughts are using SMAW process with 3/32" dia electrodes (field install) and Hastelloy X filler metal. Do you concur? Robert Upvote 0 Downvote
It is for elevated temperature to weld 1/4" 310 angle clips (that hold insulation) to G-30 Hastelloy base metal. My thoughts are using SMAW process with 3/32" dia electrodes (field install) and Hastelloy X filler metal. Do you concur? Robert
Dec 9, 2010 #4 metengr Materials Joined Oct 2, 2003 Messages 15,478 Location US Here is what you need; For shielded-metal-arc welding, G-30 alloy covered electrodes ( E N i C r M o -11; UNS W86030) are suggested. Ref http://www.haynesintl.com/pdf/h2028.pdf Upvote 0 Downvote
Here is what you need; For shielded-metal-arc welding, G-30 alloy covered electrodes ( E N i C r M o -11; UNS W86030) are suggested. Ref http://www.haynesintl.com/pdf/h2028.pdf