from the ASM High-Temperature Property Data: Ferrous Alloys, ed. Rothman, ISBN 0-87170-243-6

r.t. 200F 400F 600F
Low C steels 27.9 27.2 27.0 25.7

med C steels 29.9 29.5 28.3 26.7

all values in million psi
low C is less than 0.3%C

= = = = = = = = = = = = = = = = = = = =