Good morning all,
Here is the essentials and other variables for welding an API 15k 4130 flange/material to an A 106 grade B line piping or other P1 line piping. I've had mixed opinions about the use of FCAW for pressure piping, the ER80SNi-1, etc.
WPS is as follows:
BASE METAL: ASTM/A519 Grade 4130 Q&T API 75k material to any P1 material. thickness of 0.1875" to 1.3480"
TECHNIQUE: GTAW root and hot pass with ER80SNi-1 electrode, uphil AND FCAW fill and cap with E71T-12M electorde, uphill. no trailing shielding gas, back gouging, peening.
CONSUMABLES: EWTH-2% electrode, ER80SNi-1 consumable, E71T-12M consumable..
PRE-HEAT AND INTERPASS: 200F min. preheat, 200F-600F interpass
PWHT: 1275 hold for 1.5hr. 1hr per inch of wall thickness.....
The WPS did pass, it was written by a contractor in 1999, even though they passed, does it look like what you would recommend for a wellhead transition application to line piping?
I've heard someone say:
1. that FCAW is not recommended for pressure piping... but I think B31.3 references Section IX which inturn allows FCAW
2. that FCAW are generally used for structural and marine welding...any take on this for pressure piping???
3. they recommend ER80S-D2 TIG low allow INSTEAD of the ER80SNi-1 that was used, stating "it is used for MIG or SAW welding meets the weathering requirements of AWS D1.1 and D1.5 NOT FOR PRESSURE PIPING"
Any input will be greatly appreciated!
Thank you.
Here is the essentials and other variables for welding an API 15k 4130 flange/material to an A 106 grade B line piping or other P1 line piping. I've had mixed opinions about the use of FCAW for pressure piping, the ER80SNi-1, etc.
WPS is as follows:
BASE METAL: ASTM/A519 Grade 4130 Q&T API 75k material to any P1 material. thickness of 0.1875" to 1.3480"
TECHNIQUE: GTAW root and hot pass with ER80SNi-1 electrode, uphil AND FCAW fill and cap with E71T-12M electorde, uphill. no trailing shielding gas, back gouging, peening.
CONSUMABLES: EWTH-2% electrode, ER80SNi-1 consumable, E71T-12M consumable..
PRE-HEAT AND INTERPASS: 200F min. preheat, 200F-600F interpass
PWHT: 1275 hold for 1.5hr. 1hr per inch of wall thickness.....
The WPS did pass, it was written by a contractor in 1999, even though they passed, does it look like what you would recommend for a wellhead transition application to line piping?
I've heard someone say:
1. that FCAW is not recommended for pressure piping... but I think B31.3 references Section IX which inturn allows FCAW
2. that FCAW are generally used for structural and marine welding...any take on this for pressure piping???
3. they recommend ER80S-D2 TIG low allow INSTEAD of the ER80SNi-1 that was used, stating "it is used for MIG or SAW welding meets the weathering requirements of AWS D1.1 and D1.5 NOT FOR PRESSURE PIPING"
Any input will be greatly appreciated!