So have a gear thats a interference fit on a shaft. (by 0.08mm)
Both gear and shaft are some sort of nickel - chromium steel simular to en36a (but not necessarily so, detected composition by XRF and found closest match).

There case hardened, but not through hardened. (cutting a old gear is soft inside) But do not know the process used to harden. (suspect carburised, but its a mass produced item from a motorcycle gear box so who knows)

What to try and shrink fit assembly instead of press, But to expand the gear over the shaft would have to heat gear to a calculated 360C. Will this damage the case hardening of the gear? and any ideas as to what max temperture could be used used.
 
Replies continue below

Recommended for you

Assuming you have a steel close to EN36A, see the attachment. You have core hardness data after carburizing and another table showing the typical hardness after tempering at 200 deg C. These is a slight drop in hardness at 200 deg C.

I would limit the heat to less than 200 deg C to avoid softening the case.

 
Instead of heating the gear, why not deep freeze the shaft instead?

 

I don't think slip fittings going to fly, after all.

Heating to 200C will expand by +.04mm
Freezing with dry ice -78C contract by -.02mm
Not enough need at least .09mm difference to be desirable easy slip on.
Could freeze with liquid nitrogen at -195C will contract maybe -.05mm,
so heat and freeze potentially works, BUT would have to buy nitrogen, not worth the expense, can just press it on... (Dang! need a bigger press!)

 
and if a bigger hammer won't fix it, your problem is electrical
 
Liquid nitrogen should be relatively cheap - in central FL, the suppliers sell it by low volume amounts (less than 2 liters) for shipping bull semen.
 