Dumb question, but curious on thoughts. I know with fasteners proof is used, as the max of the elastic limit, but then we have yield which is a .2% plastic deformation, so more of a measure of when failure begins. My question is I see yield used much more commonly, but wouldn't it be better to use proof for the majority of the time, or teach it earlier?

I don't think I was even introduced to the idea of proof until later in strength of material when we studies bolts, and kind of thought that if I just designed to yield that I'd avoid failure, but that's not the case.
 
Yielding is considered failure in many applications.
 
"proof"?? do you mean ultimate (maximum) load? I've never heard "proof" used with fasteners. Its typically used in the context of things like pressure vessels, where "proof load" is used as a test load to "prove" the vessel has sufficient capability above operating pressures.
 
Yeah, I wasn't really taught it when I took my materials class for my ME degree, and don't think I even encountered it until a strength of materials class. I guess I just saw it as a very useful concept that seems to only get used for bolt connections, and felt it would have been better to introduce sooner. I'll get off my soap box now[bigsmile]
 
Yield strength is an engineering construct and not a true material property.
Since the materials that we use do not have a true straight section of the tensile curve.

We used to have to measure modulus on high strength steel wire (~300ksi UTS).
We would load to 150ksi, unload to about 35ksi, and then reload.
We would take the slope of the reload curve and we got reasonable results.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, consulting work welcomed
 
"Proof Load" exists for fasteners because the geometry is pre-defined.

For an arbitrary geometry using stress normalizes the evaluation, making it more straightforward to design or modify geometry to best match the application and constraints.
 
Hi jj1111

My understanding is proof load is used when the yield point of a material isn’t clearly defined.

“Do not worry about your problems with mathematics, I assure you mine are far greater.” Albert Einstein
 