Can you weld p22 material with a 316L material?
 
Replies continue below

Recommended for you

Can I re-phrase the question? Can you join p22 material to 316L material?

Reply,
Yes, provided a suitable filler metal is selected, like 309L or Inco 82.

 
Joining of P22 to P22 with E/ER316L filler metal should not be done, if that is your question. A high potential for weld metal cracking due to dilution exists and the dissimilar coefficients of expansion will lead to cracking during thermal cycling.

 