What would be the preferred filler metal for welding Nitronic 60 to 316L stainless Steel using the GTAW process?


RPB123
 
RPB123;
I have come across this situation where we had to deposit Nitronic 60 weld metal over a 304L substrate for increased galling resistance. For your case, if you are joining Nitronic 60 to 316L stainless, I would use a Nitronic 60 bare wire (AWS 5.9 ER218) with the GTAW process.

I attached a spec sheet for your review;

Also, keep the interpass temperature below 350 deg F during welding. I would perform a liquid penetrant test of the weld just to make sure you have no problems.
 
Thanks for the feed back and information. It was very much appreciated.

Regards,

RPB123
 