The reply to your question is yes. What is ASTM A 105N? There is an ASTM A 105, and this is what I would presume you meant in your post.
You have two options for weld filler metal to join A-182 Grade F11 to A-105 forged pipe. The ASTM A-182 Grade F11 is an ASME Section IX, P-No 4 material, while the ASTM A-105 is a P-No 1 material. You can use E7018 H4 or E8018 B2 H4 electrodes. These filler metals are for the shielded metal arc welding (SMAW) process.