Dear eng-tips,

What would happen in an already existing HAZ after performing a weld repair?

More info:
- materials SA335 P91 and A234 WP91. After NDT was performed incomplete penetration was spotted, dimension of the pipe and cap is 355,6 x 11,13 mm so re-welding form the inside is not possible.
PQRs and WPQs were properly qualified using GTAW process.

If anyone is kind enough to offer some insight I can provide more details if necessary.
 
This is due to a lack of inspection at the root of the weld.
The welder has failed and a retest is required.
The defective weld is not approved.
 
This is due to a lack of inspection at the root of the weld.
The welder has failed and a retest is required.
The defective weld is not approved.
?????????????
The welder has failed and a retest is required. ???????
 
Thank you for all your replies so far.

The welder has passed the required skill test and welded a PQR ( ASME IX) piece with succesful results ( both NDT and Mechanical testing).

The above mentioned defects were found during fabrication on the project. As r6155 said, the defect's root cause is lack of inspection.

Right now I'm trying to find the best approach to a weld repair. In my opinion, my two options are band saw the entire weld and re-bevel or grind the whole area where the defect is located ( about 20mm in lenght) and re-weld following the essential varables of the PQR.

As i find more info. regarding ways to appraoch HAZ cracking ( the entire Weld + HAZ cut out) I was left with the question if it's ok to re-weld over the existing HAZ.
 
metaleng123,
This is a question for your client.
Submit a repair request to them.
If this was discovered after PWHT it would be a different story but a localised repair (20 mm) prior to PWHT should be no problem.
What is the fabrication / construction code ?
 
@ DekDee
?????????????
The welder has failed and a retest is required. ???????
?????????????

What does ?????. Could you explain it?
Do you understand that the welder is a candidate for an award?
 
Why would 1 x repair require a retest.
That is ridiculous.
You do nothing but post negative comments.
If there was a BLOCK button I would be using it right now.
 
Yes the repair can be done. I have seen a number of such repairs been unsuccessful, finally requiring a complete cutout and reweld. You may have to make the repair area/length somewhat larger to effect a successful repair. I assume that you found the defect through RT before PWHT.
 
DekDee - ASME B31.1. I'm currently drawing up a request with an attached procedure.

weldstan - That was my idea, grind a bigger length, feather properly and re-weld. If I may, what made such repairs unsuccessful in your opinion ?
 
Overlapping HAZs are a rats nest of issues.
In some cases it doesn't matter.
In some alloys a little more heat isn't a bit deal, you test and make sure that it is OK.
But in alloys where there is precipitation it can be a nightmare.
Precipitates will grow and coarsen and this can seriously change properties.
You have to know the situation.
 
P91 welding requires great care.
Lack of penetration is a serious problem.
No inspection was performed during the root pass of the weld, and I assume the preheating and argon purging weren't inspected either.
What else happened that you don't know about?
 
@ DekDee

Once the manufacturer/ inspector has specific reason to doubt the ability of a welder, the validity of that welder gets terminated.
As clearly stated in QW-322, the welders whose validity has been revoked shall requalify.
That is, the ordinary renewal coupon is not enough to reactivate the ability.
 
Joint prep and excesive or thin root gap and land are common problems in field work, in which I am most familiar. Most of our clients only permitted one such repair and if unsuccessful, a complete cutout required. On all pipe < or = to 6" diameter, I required a complete cutout and reweld.
 
@ EdStainless, thank you for your input. In your opinion, is there a number of repairs permitted on such materials?

@ weldstan, thank you for your insight. Good to see that there is some allowance when it comes to field work. If the weld could've been accessible from the inside do you think that it would've been a better approach or would you have requested a cutout either way?
 
One of the problems with alloys like 91 is that you can't judge the creep strength of the welds based just on looking at them.
If you don't actually have data on the impact of weld repair (and re-PWHT) then caution is needed.
 
Thanks... interesting thread.
 
When accesible from the inside, like a flange to pipe weld, we would permit the repair therefrom prior to PWHT. We would have performed a dehydrogenation treatment prior to repair and initial RT..
 
I would like to thank everyone involved in this thread, it has been very helpful.
 