Using WPS with PWHT for non PWHT part

Status
Not open for further replies.

Syahar1975

Mechanical
Feb 3, 2011
224
Dear experts,

We have 1 tank with P1 Group 2 material and thickness of shell plate is 14 mm.

As required by API 650 all shell nozzles (greater than 2") and shell manholes on these shell courses must be pre-assemblied and PWHT'd before erecting at site. We have WPS with PWHT for this case.

We also have other tank with P1 Group 1 material and thickness of shell plate is 16 mm. For this shell course PWHT is not required. Can I use the above WPS with PHWT for the second case ?

Your comments is highly appreciated.

Syah

 
Replies continue below

Recommended for you

Typically you cannot do that. The WPS must be qualified with and without PWHT in order to use it for both.
 
When making the PQR coupon for the PWHT WPS, pre-plan a leftover section that you cut off and do not send out for PWHT. Keep that chunk and use it for the non-PWHT test straps. Much easier to weld one huge plate, vs. two large ones.
 
Dear DVWE , Duwe6,

Thanks for the response and suggestion.

So I will make long plate PQR with P1 Gr. 2 material. From this plate I will have 2 PQR coupons. 1 PQR will be stress relieved and the other one no stress relieved.

Than I will make 2 WPS i.e. 1 WPS with PWHT and 1 without PWHT.

Because both of tanks are using P1 material so I do not need to make 1 PQR with P1 Gr. 2 and 1 PQR with P1 Gr. 1.

Is this correct ?




 
Will you be performing impact testing?
 
Then P1 Grp 2 to P1 Grp 2 will work. Do as Duwe6 suggested with one large coupon.

P1 Grp 1 to P1 Grp 2 would only be beneficial if impact testing was required.

You will only need to write one WPS, qualified with and without PWHT. Attach both PQRs to the new WPS.
 