Hello everyone,

I'm currently in the process of designing a heat exchanger using Aspen, where the shellside carries liquid and the tubeside carries gas. For the liquid phase, we have RhoV² limits according to TEMA, but I’m unsure if there are similar guidelines for gas velocities.
From the literature I've reviewed so far, the only typical velocity range I found for gases in tubes is between 15 m/s and 30 m/s. However, I'm not sure if this range applies to my case, because the gas is condensing—not completely, but partially.
Currently, the design uses a tubeside gas velocity of 18 m/s.
Would this be considered safe and appropriate under these conditions, or should I be concerned due to the condensation aspect?
I’d appreciate any insights or recommendations from those with experience in this area.

I'm still relatively new to this type of design work, so any insights or recommended literature would be very helpful.

Thank you!
.
 
Not sure about HX's but high velocity liquid droplets in a gas stream above about 7 to 10m/sec are going to erode whatever the first thing is that it touches. Very rapidly.

Need to talk to to some HX vendors before you go modelling something which can't be built
 
What is the tube material?
Condensing streams are tricky.
Often there will be impingement protection in the form of solid rods as the first two rows in place of tubes.
In main steam condensers they run some crazy velocities but they can spread it out a lot and provide protection.
 
What is the tube material?
Condensing streams are tricky.
Often there will be impingement protection in the form of solid rods as the first two rows in place of tubes.
In main steam condensers they run some crazy velocities but they can spread it out a lot and provide protection.
The tube material can be either SS304L or Duplex 2205.

Just to confirm — impingement protection is typically intended only for the shell-side fluid, correct? Its main purpose is to protect the tube bundle from erosion caused by high-velocity flow or particles on the shell side.

In this case, the gas flows inside the tubes, which is where my concern lies. On the shell side, the liquid’s ρV² values are within acceptable limits.

Thank you for your support!
 
Not sure about HX's but high velocity liquid droplets in a gas stream above about 7 to 10m/sec are going to erode whatever the first thing is that it touches. Very rapidly.

Need to talk to to some HX vendors before you go modelling something which can't be built
My main concern is the potential for erosion inside the tubes, or any specific phenomena that may arise due to the combination of high gas velocity and droplet formation from condensation. The presence of entrained droplets at high velocity could potentially lead to erosion or other effects. As I am still gaining experience in this area, I am seeking to better understand the potential risks associated with these conditions, and would appreciate any clarification or guidance.

I’ll try to check with some vendors to make sure the design is realistic and feasible to manufacture, but before that, I’d like to better understand some of the physical phenomena that might occur under these conditions.

Thank you for your support!
 
For thermal design of and pressure drop on tubeside in partial condensors, pls refer to page 11-12 in Perry Chem Engg Handbook 7th edn. You can do a manual check of the Aspen output with these correlations.
 
2205 will resist erosion at velocities over 3m/s.
In plain clean water I have seen 2205 hold up with >25m/s flow.
The real problem in the inlet into the tubes.
Will you use a 2205 tubesheet?
Are you prepared to flare in the inlet and outlet ends of the tubes?
The 2205 will resisted droplet damage at velocities ~3x that of 304/316.
 
Tube side material should resist corrosion from condensing liquid. With such materials, velocity at 18m/sec should be okay, provided there are no erosive solids suspended in the feedgas. Overall U in this case will be constrained by shellside htc, but watch out for tubeside pressure drop.
 
2205 will resist erosion at velocities over 3m/s.
In plain clean water I have seen 2205 hold up with >25m/s flow.
The real problem in the inlet into the tubes.
Will you use a 2205 tubesheet?
Are you prepared to flare in the inlet and outlet ends of the tubes?
The 2205 will resisted droplet damage at velocities ~3x that of 304/316.
Yes, I will use 2205 for tubesheet.
As I mentioned, I'm new to this field. Is it necessary to flare both the inlet and outlet of the tubes? Is this a common practice? Does it improve the connection with the tubesheet?
 
Tube side material should resist corrosion from condensing liquid. With such materials, velocity at 18m/sec should be okay, provided there are no erosive solids suspended in the feedgas. Overall U in this case will be constrained by shellside htc, but watch out for tubeside pressure drop.
Thank you!

Yes, in this case, the overall U is limited by the shellside heat transfer coefficient. In such situations, we should aim to balance the system as much as possible, right?

As for the tubeside pressure drop, I'm working within the specified limit range.
 
The thermal designer may have picked on a higher tubeside velocity at design flow here so that at turndown, phase stratification in the tubes is still not indicated.
 
No, flaring doesn't improve joint strength.
But it greatly lower your tube side pressure drop and it go a long ways to minimize the turbulent erosion at the inlet and outlet.
 
We can't switch sides because of the corrosive nature of the tubeside fluid? I usually try to put condensing services on the shell side. Just recently we had to replace a client's condenser, and it was tube erosion. 90 fps was the best case, with all the fouling and plugs it was probably a lot higher. They stopped getting on spec product because there was so much leakage.
 
If your goal is to condense inside the tubes then you need larger diameter tubing, usually over 1.5" for this use and sometimes as large as 3".
You do this because you need to make sure that you can never get slug formation.
I can't find the paper now but in the old days Avesta published data on droplet impingement erosion.
In general the duplex SS, 6%Mo SS, and Ni alloys all did very well.
Everything else not so much.
 