Can you please advise what welding rods can be used for welding tubes (Monel) to tube sheet ( Sa 516 Gr 70)
 
Replies continue below

Recommended for you

Why don't you try google "welding Monel to Carbon Steel";- there are hips of precise informations for you.
gr2vessels
 
ERNi-1 is recommended if acceptable to meet corrosion resistance. If not butter the carbon steel side of the joint with ERNi-1 and follow with ERNiCu-7.

 