RAJMETALLURGY
Materials
Material: ASTM A352 LCB
Test coupon: 80 mm thickness, Length: 250 mm, width: 125 mm
Heat Treatment: Normalizing 930 Deg C, Quenching 910 Deg C, Tempering 650 Deg C
Mechanical Property: Yield 341.77 MPa, UTS: 506.55 MPa, Impact average 30 Joules at -46 Deg C (required 27 joules).
Simulated PWHT was carried out on test coupon after the above heat treatment NQT at 593 Deg C. Mechanical Property after this
Yield: 298 MPa, UTS: 465 MPa, Impact average 15 Joules at -46 joules
Can u pls tell me the reason for mechanical decrease after PWHT. Please help me.
Test coupon: 80 mm thickness, Length: 250 mm, width: 125 mm
Heat Treatment: Normalizing 930 Deg C, Quenching 910 Deg C, Tempering 650 Deg C
Mechanical Property: Yield 341.77 MPa, UTS: 506.55 MPa, Impact average 30 Joules at -46 Deg C (required 27 joules).
Simulated PWHT was carried out on test coupon after the above heat treatment NQT at 593 Deg C. Mechanical Property after this
Yield: 298 MPa, UTS: 465 MPa, Impact average 15 Joules at -46 joules
Can u pls tell me the reason for mechanical decrease after PWHT. Please help me.