Hi everyone. I'm currently working on manufacturing a 17-4PH casting (investment casting). But I have doubts about de test specimens from casting because this is a new project for me. The question is: How do I know where to get the test specimens from casting (no separately cast bar)? What orientation, what zones? find attached a image about piece. Could someone help me?

Likewise, how to establish the tension values for machined specimens from casting? There are always values given for separately cast bars but not for specimens cut from casting

Thanks and greetings.
 

Attachments

  • Example.jpg
    Example.jpg
    2.2 MB · Views: 9
The property requirements are the same, it doesn't matter if they are cut from the casting or separate bars.
How will the castings be heat treated?
What is the variation is wall thickness (min/max)?
What direction are the loads?
 
Thanks for your comments.

The casting will be treated by solubilization, solution and aging in accordance with AMS 5355.

The variation in wall thickness are 1 1/1" min / 2 1/4" max.

The component is subject to radial loads. Perpendicular to axial axys (find attached a image).

I have these doubts cause I've read that the test specimens cut from casting have lower values than those machined from test coupons (i.e. keel block) and I don't know the zones that I should consider to cut and machined for test specimens. This inspections is for a first article report.

Thanks and Greetings
 

Attachments

  • Example.jpg
    Example.jpg
    63.5 KB · Views: 3
I presume that the 2.25" section is thick enough to allow you to take tangential test bars out of it.
If samples from casting have lower properties, then your test blocks were either cost wrong or heat treated wrong.
The properties should be fairly consistent.
When we needed high toughness we would anneal, age (usually 1100F), and then re-anneal.
This results in grain refinement and a slight loss of strength on re-aging.
I presume that all of the machining will be done on the annealed casting with aging being done last.
 
I presume that the 2.25" section is thick enough to allow you to take tangential test bars out of it.
If samples from casting have lower properties, then your test blocks were either cost wrong or heat treated wrong.
The properties should be fairly consistent.
When we needed high toughness we would anneal, age (usually 1100F), and then re-anneal.
This results in grain refinement and a slight loss of strength on re-aging.
I presume that all of the machining will be done on the annealed casting with aging being done last.
Then would I have to expect the same mechanical properties both test specimens cut from casting (piece) and separately test specimens? I've read other comments in this forum and the mechanical properties of test specimens cut from casting (piece) are differents compared than those machined from separately cast test specimens:

If the specification is for a separately cast test specimen, but properties were determined from a specimen removed from an actual casting, then the reasons for lower the lower properties include:

1) thicker specimen from casting results in lower cooling rate, which results in larger grain/dendrite size

2) actual casting has discontinuous shape, which causes irregular flow, which causes increased porosity

Both of these factors adversely affect mechanical properties.


The casting's condition is H925 (this component is hard) and we will machining in annealed condition. We will use sand casting.
 
The variations in grain size is why we would anneal/age/anneal, in an effort to get more uniform grain size.
I hope that you don't have casting defects, that is a non-starter if you do.
 