Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

TEMPERATURE LIMIT FOR DUPLEX SS 3

Status
Not open for further replies.

gengi

Mechanical
Joined
Mar 9, 2008
Messages
20
Location
IT
Dear all,

I would be grateful if someone lets me know which is the suggestable temperature limit for the apllication of DUPLEX material ( 22% Cr - UNS N031803 - SAF 2205 )-

I learnt that, for ASME Code Div. 1 - Part II , the temperature limit is 315°C ( 600°F) ; over this temperature NO allowable stresses are available.

In addition to the tempearature limit could you please also explain the reasons of such limitation and the effect on the Duplex SS material if exposed at such high temperature ?

thanks in advance

GENGI
 
gengi;
The reason for the upper temperature limit imposed by ASME Section II subcommittee on Materials is that the duplex stainless steels develop harmful phases or precipitates at prolonged elevated temperature exposure that results in reduced strength and significantly reduced ductility.
 
The problem with higher temps is complicated. The formation of intermetallics causes significant reduction in room temperature toughness. The material will still be ductile at operating temp, but when cooled any mechanical or thermal shock may cause severe failures. There is also an associated loss of corrosion resistance.
These alloys will work for many years at 600F. I have seen tests where a couple of weeks at 630F caused serious damage.
If the highest inlet temp of your unit can ever exceed 600F (not mean metal temp) then a duplex or ferritic stainless is not a safe option.

= = = = = = = = = = = = = = = = = = = =