I am looking for the suitable material for Superheated steam (110 Barg @550 Deg C). After analyzing between P22 & P91, it is observed that P91 is best suited in terms of Rating and wall thickness point of view.
However the plant been built in a cold country, where minimum design temparature is -40 deg C, which is lower than the DBTT.
I have recieved the charpy test values for P91 @ -40C and are as under.
Standard: ASTM A-335 Gr.P91
OD X WT: 426.0mm X 32.0mm
Heat treatment: normalize and temper
Tensile strength: YS=499MPa, TS=664MPa, El=29%
(Specimen=round bar, L-direction)
Impact values: 98, 115, 66 (average 93) J/cm2 (at - 40 degC,
L-direction)
Ductility fraction: 34, 40, 29 (average 34) % (at - 40degC, L-direction).
Can I dare to use P91 material at -40C (Shutdown condition)?
However the plant been built in a cold country, where minimum design temparature is -40 deg C, which is lower than the DBTT.
I have recieved the charpy test values for P91 @ -40C and are as under.
Standard: ASTM A-335 Gr.P91
OD X WT: 426.0mm X 32.0mm
Heat treatment: normalize and temper
Tensile strength: YS=499MPa, TS=664MPa, El=29%
(Specimen=round bar, L-direction)
Impact values: 98, 115, 66 (average 93) J/cm2 (at - 40 degC,
L-direction)
Ductility fraction: 34, 40, 29 (average 34) % (at - 40degC, L-direction).
Can I dare to use P91 material at -40C (Shutdown condition)?