Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Stitch Welding 4

Status
Not open for further replies.

preusdesign

Automotive
Jun 17, 2003
3
Does anybody have experience stitch welding 24 guage 1018 cold rolled steel sheet with a mig welder?

Thanks,

Pete
 
Replies continue below

Recommended for you

Mig welding 24 ga. anything (steel, stainless) isn't going to be easy with most mig guns. With something that thin, blow-out is a big problem, but it can be done. Heli-arc/tig might be the way to go.

Flores
 
Try to weld down-hill. Try short arc with 90/10 Ar/CO2.
Go fast-kick up the volts.
 
Welding 24 ga. 1018 can be problematic. Our answer was to forgo speed of welding this type of material(Mig)for inspection/vs. quality welds.That would be Tig welding with small diameter electrodes,filler metal if required.
A good Tig welder should be able to make up the produtivity that would be lost switching from Mig to Tig welding.
We have been able to do so,with no outlay other than needed equip. for small dim. steel. Hope this was helpfull.
Tim
 
If this is an automotive application (i.e highly automated), I would look at low current Plasma Arc Welding. You get all the same advantages of GTAW (TIG or Heliarc as some say), but you get better arc starting. In some GTAW applications at low current you can blow away base metal when the arc transfers. PAW equipment is just slightly more expensive than GTAW and automation is often less difficult.

William Roth, PE, CWI
 