Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations TugboatEng on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Solid Rivet Installations - "Butt Driving"

Status
Not open for further replies.

SuperStress

Aerospace
Joined
May 5, 2003
Messages
94
Location
US
Hi folks; I haven't been around for a while... life just gets too busy.

Wil - this might be one for you.

The folks I represent are in the process of procuring a major piece of replacement structure for an aging airframe. The supplier wants to "butt drive" solid rivets (D-rivets) in the primary structure. By "butt drive", they mean to drive the rivets with the gun on the tail instead of the manufactured head. (This is NOT referring to the wonderful "NACA" rivet installations where the tails were bucked into machined countersinks...)

All of the process specs and test data support only "standard" installation, and don't specifically address this method. The OEM used the standard method during original manufacture.

The customer's position is that without test data showing equivalent hole fill and durability (as verified by testing), and without a process specification that specifically controls the proposed process, complete with Quality Assurance inspection and acceptance criteria, deviating from the tried-and-true method of rivet installation should not be allowed.

However, the customer is getting significant push-back from the supplier, a well-respected aerospace manufacturer.

Is anyone aware of any resources (old NACA data, or other public-domain resources) that might address this installation and it's interchangeability with standard installations?

If my question isn't clear, let me know...

SuperStress
 
I am going to stick my foot into this one; it may get chopped off at the ankle.

Some years ago, I read a statement that said; “The aircraft industry is the only one that allows a rivet to be driven from the factory head side. This is due to the resilience of the structure allowing it to be driven with the rivet into the bucking bar. Right now I cannot find that book. Somebody else may recognize that statement and be able to quote chapter and verse.
It would follow then, that where a structure is not resilient, like a heavy frame or cross member, that conventional riveting (From the shop head or buck tail side) would be preferred. The rational for driving from the factory head side is to ensure that the head is fully seated against the part it is being driven into. If the part has too much inertia it is very difficult to form the buck tail.
The easier solution then, is to put the bucking bar against the factory head of the rivet, and buck the tail. The dis advantage of this is that if the bucking bar is not perfectly held the rivet can creep back a little as it is being formed and leave a gap under the head.
This makes the QA inspectors day as he crawls over your job brandishing his feeler gauge.


 
"The dis advantage of this is that if the bucking bar is not perfectly held the rivet can creep back a little as it is being formed and leave a gap under the head."

This has been my experience.
 
Im not sure about a readily available NACA datasheet or public domain resources but I have found a reference in Airbus SRM about this. (A340 51-42-11)

I think they permit this principle but under the category of hand hammering.

-support the manufactured with a correct rivet set/dolly if csk
-hold a dolly against the upset head and hit it with hammer
(few and heavy strikes are necessary to avoid hardening the rivet)
-strike more if necessary to achieve correct shape of upset head.

I think its the same principle.
but this reference is used for small repairs and involves few rivets.

my opinion/interpretation:
they said only for "few rivets" and "small repairs" bcoz imagine the amount of workload/energy needed to accomplish this with primary structure (by hand).

defense: use the principle and automate the process by using a riveting gun. (riveting gun=pneumatic hammer)

 
Super Stress... Please, advise...

Protruding head [MS20470 brazier style]: resulting-in protruding heads on both sides??

Flush-tension head [MS20426 100-deg style] into a csk or dimple-into-csk: resulting-in flush one-side and protruding opp side??

Flush-shear head [NAS1097 style] into a csk or into double csks: resulting in flush one-side and protruding opp side; or flush both sides??

What temper are the "D" rivets driven????
"D" [2017] rivets can be driven "hard" [with a chem-conversion-coating OR anodized finish]; or can be driven "soft" ["ice-box" temper (-W), with an anodize finish, ONLY]. Per NAS523, "D" rivets driven "hard" attain the -T4 temper; while "D" rivets driven "soft" [-W, as quenched] attain the -T31 temper (in no-more-than 96-hours). Minor difference, structurally, in the long-term... but a HUGE difference in installation ease and quality [especially for larger diameter rivets].

I will check some older riveting source-data, but I am NOT comfortable with reverse driving brazier head rivets without the proper sets. Issue may be fuzzier with flush head rivets.

NOTE. Your shop should have strict process documentation that rigidly establishes for riveting methodology that is non-standard. IF there are NO rigid shop procedures [training?] in place then "You get-what-you-get"... and riveter-to-riveter [random] variations can enter the picture.

Hole (or hole/csk) preparation???
As usual, hole preparation [IE: straightness, perpendicularity, roundness, roughness, deburring, inner-laminar chipping, +plus all countersink issues, etc] can make a BIG difference... grossly affecting installation soundness.

NOTE.
IF installation processes are standardized (and rigorously enforced), then each technician can execute a simple series of riveting coupons that will be: (a) shear and tension tested to verify static strength; and (b) metallurgically sectioned [thru several fasteners] looking for micro-installation quality and grain flow, relative to "nominally shot" (conventionally riveted) coupons [also sectioned].

Later today/tomorrow, I will look at some old riveting tests that I have for reverse riveting practices.

NOTE.
I suspect that protruding flat-head rivets [IE: AN442] were in use for a long time [40's, 50s], due to ease of shooting from either side.

Regards, Wil Taylor

Trust - But Verify!

We believe to be true what we prefer to be true.

For those who believe, no proof is required; for those who cannot believe, no proof is possible.
 
Wil,

Here's what I know...

1/4" MS20470D (BM8) rivets.

Temper: driven hard.

Hole prep: Good hole prep and quality control per standard shop practices.

The primary concern is about gapping and consistent residual clamp-up. Hole fill on the manufactured head side is generally constrained by the manufactured head so the benefit of hole fill is less than on the buck-tail side by around 5-10% (in terms of stress) depending on the specific drive (standard/overdrive), fastener style, material, etc.

If gapping is more likely with this installation, and the gapping is not caught, overall joint quality will suffer and lead to premature fatigue cracks. Additionally, varying degrees of hole fill along a fastener line will lead to non-uniform load transfer and hot-spots. Driving the head into the structure reduces the chance of gapping even if the person on the bucking bar pushes the rivet out slightly to identify which rivet he/she is ready to buck and the driver hits the trigger too soon before pushing the set against the head/structure. On the first few hits the gun will still drive the heard toward the structure because there typically hasn't been enough expansion to preclude shank movement in the hole. This reduces the probability of gapping.

I think we are at the point where we have convinced the supplier to install per approved procedures for future units. The question now is whether or not we have a potential quality issue on previously-produced items. We may not be able to address this analytically... The relative fatigue performance of the joint is irrelevant if we can't ascertain the quality of the install (head gapping).

Still, if you have any data that suggests relative performance of joints with rivets bucked from head vs. tail side, it would be useful.

Thanks for your time!

SuperStress
 
my mention mistiming between the bucker and the driver ... driving the manufactured head will set the rivet if the bucking bar is slow into position. driving of the shop head ... this'll be a problem, no?

the other point mentioned is the bucking bar would need a recess for the protruding head.
 
SuperStress...

BM8's will be an SOB to drive with a 3X rivet gun in any conventional [gun-on-head] sense [not to mention extremely loud and possibly damaging to the structure].

I suspect that the mechanics want to reverse drive to ensure max gun-energy directed to deform the tail. If this is the reason, then stop the presses... as You indicate there will be hole-fill issues galore.

IF this is the case, then what has happened is that the shop is circumventing rivet conventional installation protocol in-favor-of "just getting the job done [any-way they can]". This is a shabby way to run an aerospace company.

IF the 1/4D rivets MUST be driven hard, then the only practical and reliable methods are (a) manually-guided hand-squeezing using a portable long-jaw hydraulic unit; or (b) a gantry type automated squeeze-unit, IE: as used for automated skin panel Assy [etc].

Otherwise the shop needs to get intimate with the ice-box ["-w" temper] rivet installation technique. Guys tell me that D and DD rivets up-to/slightly above 3/8"-Dia shoot much like 1/8"-to-5/32"-Dia hard rivets "nice and soft... like butter". Rivet installation quality is very good. The only problem here is that the shop REALLY needs to understand how the process works; and that D rivets with an anodized finish [to survive solution HT] may be hard to find.

Regards, Wil Taylor

Trust - But Verify!

We believe to be true what we prefer to be true.

For those who believe, no proof is required; for those who cannot believe, no proof is possible.
 
Wil and super stress,
"" I suspect that the mechanics want to reverse drive to ensure max gun-energy directed to deform the tail. If this is the reason, then stop the presses... as You indicate there will be hole-fill issues galore.""
They will be mushrooming the tail without swelling the shank.

On a 1/4" dia rivet the installer should be using at least a 5X gun. Most 3X guns max out at a 3/16" dia rivet with a 470D
I would feel happier using a 7X slow hitter.
Quenched rivets will be a lot easier to shoot if the shop can stay within the "out times" Then on a 1/4" rivet you could get by with a 5X hammer without any problem.
B.E.
 
Can some point me to a "coupon test method" for rivets. Would be nice to confirm (shear/tension) mechanical properties on batches of rivets (i.e. AN4 washer, two sheets 0.100", another AN4 washer... then either pull for shear test, or form into a delta shape and pull to failure for tension.

I'm thinking of a pull test. 38,000 psi rivet spec, but on a AN3 diameter should pull with more than 26 pounds of force. Simple newsletter approach for the local EAA chapter on how to make sure you have good techniques.



 
Get yourself a back setting tool. The rivet head is held with the gun and snap (with a bit of tape on to prevent smiling the rivet) (or a machined block) as per usual and with the tool (looks like a straight snap but with a nylon sleeve to stop the face moving off the rivet)form the rivet tail. I agree DD rivets should be formed in the "ice box" condition (3/16 and above).
Good luck
 
First time on the forum....

I have a question. I'm using MS20426 rivets but I'm being told to install the rivets per NASM47195. That spec calls out for the (MS)20600, 20601, and 20605 rivets. These rivets are the pull stem type while the MS20426 is a solid rivet.

Would the NASM47196 be a more appropriate spec to be used for the MS20426 rivets? Keep in mind I have the flush mounted type.

Thanks for your help.
 
Keithster...

You are absolutely correct.

Regards, Wil Taylor

Trust - But Verify!

We believe to be true what we prefer to be true.

For those who believe, no proof is required; for those who cannot believe, no proof is possible.
 