dieselofdog

Materials
Joined
Feb 11, 2014
Messages
28
Location
AU
I am going to run a PQR joining 625 (solution annealed) to itself using NiCrMo-3 filler. GTAW in the root and deposit 6mm of weld metal. Then GMAW-Pulse for the remainder. The test plates will be 40mm thick and double U Preps will be machined at 60 deg included.

What shielding gas is recommended for GMAW-Pulse process? I believe 100% Ar can be used but would a He blend be better for penetration and avoiding lack of fusion defects and toe wetting?
 
GMAW pulse should use 90% Ar- 7.5% He -2.5% CO2 or 75% He-25% Ar
 
I haven't seen people running a mix with CO2, but Ar-He blends are very common.
I have seen a lot of 75% Ar-25% He used.
He helps with heat transfer, but I don't think that will be an issue with your process.


= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 
Argon for TIG, Argon-He mixtures. We've used 60He-40Ar and the mixtures provided by metengr and Ed for GMAW.
 
we use 75% He-25% Ar
 