Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Self cementing properties of calcrete 2

Status
Not open for further replies.

gesi

Civil/Environmental
Apr 30, 2007
4
How can i evaluate by testing the self cementing properties of calcrete gravel?
 
Replies continue below

Recommended for you

I would suggest one of two methods:

Compact the material into a CBR mold with its moisture content at around 10 to 11 percent by weight. Soak the material,in the mold, for at least 24 hours, then carefully extract from the mold as a cylindrical specimen and allow to dry. Run an unconfined compressive strength test on the material to determine its compressive strength. Compare to similar, non-cementing materials.

The second method is similar except you will simply place the material into a 6" diameter by 12" tall compressive strength test mold and moderately compact it in 3 lifts. We the material and allow to soak for at least 24 hours. Pour off all water, allow to air dry and then test in unconfined compression. Compare to other similar, but non-cementing materials.

If in either case your unconfined compressive strength exceeds about 200 psi, you are getting some significant cementation.

Good luck.
 