Aug 12, 2010 #1 Guest102023 Materials Joined Feb 11, 2010 Messages 1,523 Location CA I want to weld T11 boiler tube to carbon steel tube, WT = 0.180" or less. I need to know the possible preheat and PWHT reqirements in Section I, which I do not have access to. Thanks.
I want to weld T11 boiler tube to carbon steel tube, WT = 0.180" or less. I need to know the possible preheat and PWHT reqirements in Section I, which I do not have access to. Thanks.
Aug 12, 2010 1 #2 stanweld Materials Joined May 9, 2003 Messages 2,906 Location US 250 F (120 C) per Table PW-39, for P No. 4, General Notes (a)(1)(c). Upvote 0 Downvote
Aug 12, 2010 Thread starter #3 Guest102023 Materials Joined Feb 11, 2010 Messages 1,523 Location CA Thanks, Stanweld. Upvote 0 Downvote
Aug 12, 2010 #4 stanweld Materials Joined May 9, 2003 Messages 2,906 Location US With wall thickness up to 0.165" (max) and max OD of 1.5", preheat is not mandated when buttwelded with the GTAW process per same note. Upvote 0 Downvote
With wall thickness up to 0.165" (max) and max OD of 1.5", preheat is not mandated when buttwelded with the GTAW process per same note.
Aug 29, 2010 #5 pandithan Mechanical Joined May 20, 2001 Messages 101 Location IN No Preheat is required for this 4.5mm thick Upvote 0 Downvote