Eng-Tips is the largest forum for Engineering Professionals on the Internet.

Members share and learn making Eng-Tips Forums the best source of engineering information on the Internet!

  • Congratulations dmapguru on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Rubber hose recipe help ???? 3

Status
Not open for further replies.

Terikanli10

Industrial
Joined
Jun 18, 2019
Messages
16
Location
TR
Hello friends, please write me rubber hose recipes. I'm gonna build a fuel hose, please.
 
What kind of fuel, with what additives? What is the usage temperature? Ozone? Sunlight/UV?
 
friends, I need a recipe for fuel hose, garden hose and vehicle wick
 
Rubber dough recipe
Phr
Rubber 100
Çinko oksit. 5
Fed N 550. 8
as......
 
What fuel - diesel or petrol/gasoline?

What is a vehicle wick?

forumtowers.com
 
Probably the lowest cost garden hose I can think of would be made from extruded LDPE but if you want to make it from rubber then I suggest the following:

Natural rubber (grade TC20) 100.00 phr
Calcium carbonate 100.00 phr
Carbon black N550 8.00 phr
Process oil 10.00 phr
Zinc oxide 4.00 phr
Stearic acid 1.00 phr
Santoflex 13 1.50 phr
Sunproof Improved wax 2.50 phr
Sulfur 3.00 phr
MBTS 1.00 phr
TMTD 0.15 phr

forumtowers.com
 
What oil do I need to use for epdm brother
 
EPDM must not be used with mineral oil. It works great for garden hose applications.
 
Well, do you write epdm rubber recipe for garden hose
Römörkor
 
OK, here's an EPDM-based formulation:

EPDM 100.00phr
Carbon black grade N550 100.00phr
Carbon black grade N762 50.00phr
Calcium carbonate 75.00phr
Zinc oxide 5.00phr
Stearic acid 0.50phr
Paraffinic process oil 100.00phr
TMTD 0.60phr
ZDBC 1.50phr
MBT 2.00phr
Sulfur 0.50phr

Thanks for the star whoever gave it me.[thumbsup2]