Hi all,

How can I calculate the hardness (ShoreA) of a silicone rubber compound? I have 70 Sh and 40 Sh base rubber, peroxide catalyst, and quartz as filler. I would like to obtain 65 Sh rubber. Is there any equation to estimate the hardness before producing?
İf i would mix the same amount of 70Sh and 40Sh base rubber (let’s say 10 kg per each base) how much filler am i going to need to reach the 65 shore value?

Thanks,
 
Replies continue below

Recommended for you

Hi,

that is no rocket science.

Most silicone bases are additive concerning hardness, chemists call it mixing cross --> 5 parts of 40 Shore and 25 parts of 70 Shore.

(5x40 + 25*70)/30 = 65

Ground quartz has quite low influence on hardness (appr. +2 pts. per 10 parts of filler). Quartz is not so healthy stuff, look for a ready batch from your silicone supplier.
Quartz reduces Tensile strength , so check your specification before.

Remark: If you mix 40 and 70 1:1, result will be 55, hence you need appr. 50 parts of quartz. It is possible, it is cheap, but it is very crumbly stuff with low mechanicals.

Peroxide: Some silicones show very different Shore A values with different peroxides and all nominal hardness values are +/-5 usually, so better test hardness of your "40" and "70" with the intended peroxide type first before calculating final hardness.

Or simply do trial and error ;-(( Let us know your results.

Good luck.