Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations cowski on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Rubber curing systems

Status
Not open for further replies.

samster06

Mechanical
Apr 22, 2006
1
Can someone please provide me with a list of rubber curing systems (sulfur-based, peroxide-based, etc) and how each applies to the different elastomeric families (FKM, EPDM, VMQ, etc)?
 
Replies continue below

Recommended for you

Elastomer General Purpose Fast cure


NR TBBS 0,5 MBTS 0,5
TMTD 0,2 ZMDC 0,3
S 2,7 S 2,0



SBR MBTS 1,5 TBBS 1,0
CUMATE 0,2 CUMATE 0,3
S 2,0 S 1,7



NBR MBTS 2,0 MBT 1,5
TMTD 1,0 ZMDC 1,5
S 1,5 S 1,5


EPDM MBT 1,5 DPTT 0,8
TMTD 1,0 TEDC 0,8
TETD 0,5 TMTD 0,8
S 1,5 MBT 1,5
S 2,0


IIR MBT 1,0 MBTS 1,0
TMTD 2,0 CADMATE 1,0
S 1,5 TEDC 1,0
S 2,0


CR DOTG 1,0 VANAX PML 1,5
TMTM 1,0 CaO 2,0
S 1,0




CSM TMTD 2,0 DPTT 2,0
S 1,0
 
The R. T, Vanderbilt Handbook would be the best source for this information. There are many, many curing systems and it lists the most common for each type of polymer. appliction information is also included. I believe the Handbook is available "on line"==you can run a search via Dogpile, Google, etc
 