Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations JAE on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Rubber curing systems

Status
Not open for further replies.

samster06

Mechanical
Joined
Apr 22, 2006
Messages
1
Location
US
Can someone please provide me with a list of rubber curing systems (sulfur-based, peroxide-based, etc) and how each applies to the different elastomeric families (FKM, EPDM, VMQ, etc)?
 
Elastomer General Purpose Fast cure


NR TBBS 0,5 MBTS 0,5
TMTD 0,2 ZMDC 0,3
S 2,7 S 2,0



SBR MBTS 1,5 TBBS 1,0
CUMATE 0,2 CUMATE 0,3
S 2,0 S 1,7



NBR MBTS 2,0 MBT 1,5
TMTD 1,0 ZMDC 1,5
S 1,5 S 1,5


EPDM MBT 1,5 DPTT 0,8
TMTD 1,0 TEDC 0,8
TETD 0,5 TMTD 0,8
S 1,5 MBT 1,5
S 2,0


IIR MBT 1,0 MBTS 1,0
TMTD 2,0 CADMATE 1,0
S 1,5 TEDC 1,0
S 2,0


CR DOTG 1,0 VANAX PML 1,5
TMTM 1,0 CaO 2,0
S 1,0




CSM TMTD 2,0 DPTT 2,0
S 1,0
 
The R. T, Vanderbilt Handbook would be the best source for this information. There are many, many curing systems and it lists the most common for each type of polymer. appliction information is also included. I believe the Handbook is available "on line"==you can run a search via Dogpile, Google, etc
 