Hello friends, please help me

If i Have to qualify a procedure whit thickness 10 mm. Smaw with impact test

Wich is mandatory to define range thickness?

Asme b31.3 tab. 323.3.1 A-5 or Asme Ix 403.6 and 451

Minimum qualified it's 10mm, 403.6 asme IX. Ok, but maximun it's T+6mm like Asme b31.3 tab. 323.3.1 A-5 or 2T like QW451????

Thanks a lot!!
 
If the code of construction is ASME B31.3, impact qualification and thickness ranges are followed over Section IX.
 
This is the third place you have submitted the same (misspelled and ungrammatical) request. Do not duplicate threads in different forums.
 
Ok racookpe1978

I'm sorry.
 
Thanks
But i need be sure the Maximum thickness qualified. If my procedure use 10mm i know the min by qw 403.6 its 10mm, but the max??? Its 10+6mm following Asme b31.3 323.3.1 or its 20mm following Asme Ix qw451???

:))

 
If you originally qualified your WPS to Section IX, QW-403.6, you qualify to the minimum coupon thickness only as indicated below in QW-403.6

The minimum base metal thickness qualified is the thickness of the test coupon T or 5/8 in.
(16 mm), whichever is less. However, where T is less than 1/4 in. (6 mm), the minimum thickness qualified is 1/2T.

The maximum thickness is based on the weld deposit thickness range qualified for the WPS.

If B31.3 code is invoked, Table 323.3.1 A-5 is followed specifically for impact testing of welds, thickness range and number of impact tests.
 
"A" asks min thickness qualified
"C" asks range qualified

Asme B31.3
With impact test
 
Per B31.3, your PQR on 10 mm pipe, qualifies the thickness range from 5 mm to 16mm for the pipe subject to impact testing.
 