Our heat treating contractor just sent a unit back. Reviewing the charts, we found that the unit was post weld heat treated at 1250°F instead of the specified 1150°F.

The item is a T-strainer - constructed of carbon steel body and flanges.

Will this cause any problems?
 
Replies continue below

Recommended for you

No. This temperature is below the lower critical transformation temperature for carbon steel.
 
In general, I agree with metengr. Time at 1250 F and somewhat greater temperature may reduce tensile strength of some of the very low carbon medium manganese weld filler metals below their stated minimums. I have certainly seen it occur at 1275 F and 1300 F.
 